Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy
Material This alloy has good workability, very good corrosion resistance, high fatigue strength,
Notes: weldability, and moderate strength. This leads to its use in aircraft fuel/oil lines, fuel
tanks, other transportation areas, sheet metal work, appliances and lighting, wire, and
rivets.

Data points with the AA note have been provided by the Aluminum Association, Inc.
and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.
Key Words: UNS A95052; ISO AlMg2.5; Aluminium 5052-H36; AA5052-H36
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your
listing to this material.
Printer friendly version Download as PDF Download to Excel
Add to Folder:
(requires Excel and Windows)
Export data to your CAD/FEA program

Physical Metric English Comments


Properties
Density 2.68 g/cc 0.0968 lb/in³ AA; Typical

Mechanical Metric English Comments


Properties
Hardness, 73.0 73.0 AA; Typical; 500 g load; 10 mm ball
Brinell
Hardness, 96.0 96.0 Converted from Brinell Hardness Value
Knoop
Hardness, 83.0 83.0 Converted from Brinell Hardness Value
Vickers
Ultimate Tensile 276 MPa 40.0 ksi AA; Typical
Strength
Tensile Yield 241 MPa 35.0 ksi AA; Typical
Strength
Elongation at 8.00 % 8.00 % AA; Typical; 1/16 in. (1.6 mm)
Break Thickness
10.0 % 10.0 % AA; Typical; 1/2 in. (12.7 mm) Diameter
Modulus of 70.3 GPa 10200 ksi AA; Typical; Average of tension and
Elasticity compression. Compression modulus is
about 2% greater than tensile modulus.
Poissons Ratio 0.330 0.330
Fatigue Strength 131 MPa 19000 psi completely reversed stress; RR Moore
@# of Cycles 5.00e+8 @# of Cycles 5.00e+8 machine/specimen
Shear Modulus 25.9 GPa 3760 ksi
Shear Strength 159 MPa 23000 psi AA; Typical

Electrical Metric English Comments


Properties
Electrical 0.00000499 ohm-cm 0.00000499 ohm-cm AA; Typical at 68°F
Resistivity

Thermal Metric English Comments


Properties
CTE, linear 68°F 23.8 µm/m-°C 13.2 µin/in-°F AA; Typical; Average over 68-212°F
range.
CTE, linear 25.7 µm/m-°C 14.3 µin/in-°F Average over the range 20-300ºC
250°C
Specific Heat 0.880 J/g-°C 0.210 BTU/lb-°F Estimated from trends in similar Al
Capacity alloys.
Thermal 138 W/m-K 960 BTU-in/hr-ft²-°F AA; Typical at 77°F
Conductivity
Melting Point 607.2 - 649 °C 1125 - 1200 °F AA; Typical range based on typical
composition for wrought products 1/4
inch thickness or greater
Solidus 607.2 °C 1125 °F AA; Typical
Liquidus 649 °C 1200 °F AA; Typical

Processing Metric English Comments


Properties
Annealing 343 °C 650 °F holding at temperature not required
Temperature
Hot-Working 260 - 510 °C 500 - 950 °F
Temperature

Material Metric English Comments


Components
Properties
Aluminum, Al 95.7 - 97.7 % 95.7 - 97.7 % As remainder
Chromium, Cr 0.150 - 0.350 % 0.150 - 0.350 %
Copper, Cu <= 0.100 % <= 0.100 %
Iron, Fe <= 0.400 % <= 0.400 %
Magnesium, Mg 2.20 - 2.80 % 2.20 - 2.80 %
Manganese, Mn <= 0.100 % <= 0.100 %
Other, each <= 0.0500 % <= 0.0500 %
Other, total <= 0.150 % <= 0.150 %
Silicon, Si <= 0.250 % <= 0.250 %
Zinc, Zn <= 0.100 % <= 0.100

Aluminum Weldalite 049-T6

Categories: Metal; Nonferrous Metal; Aluminum Alloy; Other Wrought Al Alloy


Material Notes: Weldalite® was developed by Lockheed Martin and is produced under license
by McCook Metals LLC, and Alcoa.
Key Words: Aluminium; Al-Li; Aluminum Lithium Alloy, Al 2195
Vendors: No vendors are listed for this material. Please click here if you are a supplier
and would like information on how to add your listing to this material.
Printer friendly version Download as PDF Download to
Add to Folder:
Excel (requires Excel and Windows)
Export data to your CAD/FEA program

Physical Properties Metric English Comments


Density 2.60 g/cc 0.0939 lb/in³ Estimated from trends in similar Al
alloys.

Mechanical Properties Metric English Comments


Tensile Strength, Ultimate 720 MPa 104000 psi 9 mm Extruded Plate
Tensile Strength, Yield 680 MPa 98600 psi 9 mm Extruded Plate
Elongation at Break 4.00 % 4.00 % In 5 cm; 9 mm Extruded Plate
Fracture Toughness 30.0 MPa-m½ 27.3 ksi-in½ K(IC) in L-T orientation (temper T6E4)
Shear Strength 420 MPa 60900 psi

Material Components Metric English Comments


Properties
Aluminum, Al 92.0 % 92.0 % As remainder
Copper, Cu 5.40 % 5.40 %
Lithium, Li 1.30 % 1.30 %
Magnesium, Mg 0.400 % 0.400 %
Silver, Ag 0.400 % 0.400 %
Zirconium, Zr 0.140 % 0.140 %

References for this datasheet.

Aluminum, Al
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Pure Element
Material Aluminum is a silver-colored, low density (2.7 g/cc) metal that finds use in a huge
Notes: variety of commercial applications. Unalloyed aluminum is ductile, exhibits moderate
strength, and is very resistant to corrosion under most circumstances. Aluminum can
be dramatically strengthened by the addition of appropriate alloying elements (Cu, Mg,
Mn, Si, etc.) and subsequent heat/work treatments. Aluminum is commonly used in
both wrought and cast forms.

The low density of aluminum results in its extensive use in the aerospace industry, and
in other transportation fields. Its resistance to corrosion leads to its use in food and
chemical handling (cookware, pressure vessels, etc.) and to architectural uses.

Over 1175 Al alloys are listed in MatWeb. Aluminum 1199 is the highest purity
(99.99% Al min.) commercially available in structural form.
Vendors: No vendors are listed for this material. Please click here if you are a supplier and
would like information on how to add your listing to this material.
Printer friendly version Download as PDF Download to Excel
Add to Folder:
(requires Excel and Windows)
Export data to your CAD/FEA program

Physical Metric English Comments


Properties
Density 2.6989 g/cc 0.097504 lb/in³

Mechanical Metric English Comments


Properties
Hardness, 15.0 15.0 Annealed
Vickers
Modulus of 68.0 GPa 9860 ksi
Elasticity
Shear Modulus 25.0 GPa 3630 ksi
Electrical Metric English Comments
Properties
Electrical 0.00000270 ohm-cm 0.00000270 ohm-cm
Resistivity
Magnetic 6.00e-7 6.00e-7 cgs/g
Susceptibility
Critical Magnetic 101.9 - 107.9 101.9 - 107.9
Field Strength,
Oersted
Critical 1.73 - 1.77 K 1.73 - 1.77 K
Superconducting
Temperature

Thermal Metric English Comments


Properties
Heat of Fusion 386.9 J/g 166.4 BTU/lb
CTE, linear 24.0 µm/m-°C 13.3 µin/in-°F over the range 20-100ºC
20°C
CTE, linear 25.5 µm/m-°C 14.2 µin/in-°F over the range 20-300ºC
250°C
CTE, linear 27.4 µm/m-°C 15.2 µin/in-°F over the range 20-500ºC
500°C
Specific Heat 0.900 J/g-°C 0.215 BTU/lb-°F
Capacity
Thermal 210 W/m-K 1460 BTU-in/hr-ft²-°F
Conductivity
Melting Point 660.37 °C 1220.7 °F

Optical Metric English Comments


Properties
Emissivity (0-1) 0.200 - 0.300 0.200 - 0.300 strongly oxidized
0.0500 0.0500 polished 50-500ºC
Reflection 0.900 0.900 tungsten light
Coefficient,
Visible (0-1)

Material Metric English Comments


Components
Properties
Aluminum, Al 100 % 100 %

Descriptive Properties
CAS Number 7429-90-5

References for this datasheet.

Aluminum 1050-H14
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 1000 Series Aluminum
Material Data points with the AA note have been provided by the Aluminum Association, Inc.
Notes: and are NOT FOR DESIGN.

Composition Notes:
The aluminum content for unalloyed aluminum not made by a refining process is the
difference between 100.00 percent and the sum of all other analyzed metallic elements
present in amounts of 0.010 percent of more each, expressed to the second decimal
before determining the sum. For alloys and unalloyed aluminum not made by a refining
process, when the specified maximum limit is 0.XX, an observed value or a calculated
value greater than 0.005 but less than 0.010% is rounded off and shown as " less than
0.01%".
Composition information provided by the Aluminum Association and is not for design.
Key Words: Aluminium 1050-H14; UNS A91050; NF A5 (France); DIN Al99.5; AA1050-H14, ASTM
B491; BS 1B (UK); CSA 9950 (Canada); ASTM B491
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your
listing to this material.
Printer friendly version Download as PDF Download to Excel
Add to Folder:
(requires Excel and Windows)
Export data to your CAD/FEA program

Physical Metric English Comments


Properties
Density 2.705 g/cc 0.09772 lb/in³ AA; Typical

Mechanical Metric English Comments


Properties
Hardness, 30.0 30.0 500 kg load with 10 mm ball. Calculated
Brinell value.
Tensile 110 MPa 16000 psi
Strength,
Ultimate
Tensile 103 MPa 14900 psi
Strength, Yield
Elongation at 10.0 % 10.0 % In 5 cm; Sample 1.6 mm thick
Break
Modulus of 69.0 GPa 10000 ksi In Tension; Compressive Modulus is
Elasticity about 2% higher
Poissons Ratio 0.330 0.330
Shear Modulus 26.0 GPa 3770 ksi Estimated from similar Al alloys.
Shear Strength 69.0 MPa 10000 psi

Electrical Metric English Comments


Properties
Electrical 0.00000290 ohm-cm 0.00000290 ohm-cm
Resistivity

Thermal Metric English Comments


Properties
Heat of Fusion 390 J/g 168 BTU/lb
CTE, linear 23.6 µm/m-°C 13.1 µin/in-°F 20-100ºC
20°C
CTE, linear 25.5 µm/m-°C 14.2 µin/in-°F Average over the range 20-300ºC
250°C
Specific Heat 0.900 J/g-°C 0.215 BTU/lb-°F
Capacity
Thermal 227 W/m-K 1580 BTU-in/hr-ft²-°F
Conductivity
Melting Point 646 - 657 °C 1190 - 1210 °F
Solidus 646 °C 1190 °F
Liquidus 657 °C 1210 °F

Material Metric English Comments


Components
Properties
Aluminum, Al >= 99.5 % >= 99.5 %
Copper, Cu <= 0.0500 % <= 0.0500 %
Iron, Fe <= 0.400 % <= 0.400 %
Magnesium, Mg <= 0.0500 % <= 0.0500 %
Manganese, Mn <= 0.0500 % <= 0.0500 %
Other, each <= 0.0300 % <= 0.0300 %
Silicon, Si <= 0.250 % <= 0.250 %
Titanium, Ti <= 0.0300 % <= 0.0300 %
Vanadium, V <= 0.0500 % <= 0.0500 %
Zinc, Zn <= 0.0500 % <= 0.0500 %

References for this datasheet.